I’m not familiar with jp vest but when I press I do the following.
I never use debubblizer. I find too many issues with it. Lots of orange peel texture after pressing.
After I invest, I wait until the ring is completely dry. I don’t work in a ‘rushed’ environment so I don’t have the need to fast press.
I place the invested ring into a cold furnace and raise temp to 400C, then 25 minute hold. Then raise to final temp, 850C and hold for another 45 minutes. Then place into pressing furnace.
it works great for me. RARELY have mispress issues or cracked rings. YMMV.
Thomas.
thanks for the reply
I Did not use debubblizer for this press, also was not in a hurry environment, it was a test press to see how it works.
But yes the burnout method has to do something with it, i mhave to change it.