Were an all porcelain lab. But I have a case I need to build pfm's on. So were going to use our EX3 kit. I am too busy to do my DD on a great alloy for the EX3. So maybe I should just get an ounce of whatever your already using that works well...

Something precious.
 
ICONDENTAL

ICONDENTAL

Member
Full Member
Messages
87
Reaction score
4
For EX3 NORITAKE.if you like to use yellow alloys ARGEDENT bio 89pf.but if you like white alloys ARGEDENT 51sf. is good for argedent 51sf Oxidation Procedure: 650-1010°C, Vacuum, no hold, remove oxide and for ARGEDENT bio 89sfOxidation Procedure: 650-980°C, no hold, Do not remove oxide, no vacuum hot plate recommended . and also make sure to use "poba" as your first opaque. good luck.
 