I've had good luck with proform's duals laminates, hard on one side, soft on the other.
Duplicate models,
trim dup model to horseshoe,
PreHeat the machine to red-hot,
place laminate in frame softside up and heat until glaze (1:30-2:00 minutes),
Flip laminate to hardside up and heat 10 -15 seconds (it'll blister if you overheat),
Lower frame and turn on vacuum motor for a good minute,
bench cool for 10 or dunk in water to cool,
trim
Duplicate models,
trim dup model to horseshoe,
PreHeat the machine to red-hot,
place laminate in frame softside up and heat until glaze (1:30-2:00 minutes),
Flip laminate to hardside up and heat 10 -15 seconds (it'll blister if you overheat),
Lower frame and turn on vacuum motor for a good minute,
bench cool for 10 or dunk in water to cool,
trim